Linear polyacrylamide is made by polymerising a 5% acrylamide
solution in 40mM Tris, 20mM Na acetate, 1mM EDTA pH7.8 together with
1/100 vol of 10% ammonium persulphate and 1/1000 vol. TEMED. When the
solution becomes viscous (about 15-30mins) ppt polymer with 2.5volumes
EtOH, centrifuge and redissolve pellet in 20 vol. water O/N. Use 10ul
(25ug) per EtOH pptation.